Alloy 31 (UNS N08031) bat Hastelloy C276 (UNS N10276) nan asid fòtman oksidan, epi li koute apeprè mwatye nan matyè premyè.Nan bouyi tès asid nitrique pibliye pa pwodiktè yo, Alloy 31 pèdi apeprè 0.1 mm / an metal, pandan y ap C276 pèdi apeprè 22 mm / y. Alloy 31 pote 27% CHROMIUM; C276 pote 16%. Chromium bati fim pwoteksyon ki asid oksidant pa ka kraze.

 

C276 se toujou pi bon chwalè yon oksidan melanje ak asid idroklorik, lè tanperati konsepsyon an pi wo pase 427 degre (800 degre F), oswa lè pitting risk ekstrèm. Estimasyon 2026 nou an ki genyen-metal mete Alloy 31 nan apeprè 10,70 USD/kg kont 21,40 USD/kg pou C276.

 

Alloy 31 vs Hastelloy C276

 

Yon ti koutje sou alyaj 31 vs C276

 

Dimansyon

Alyaj 31 (N08031)

Hastelloy C276 (N10276)

Edge

Kwòm / Molybdène

27% Cr / 6.5% Mo

16% Cr / 16% Mo

Sa depann de asid

Bouyi asid nitrique

0.1 mm/a (Tès Huey-tip)

22.12 mm/y (65% asid)

Alyaj 31

Asid idroklorik

Jiska apeprè 8% nan tanperati chanm

Jiska 20% ak pi wo, jiska 79 degre

C276

Pitting grav (lanmò vèt)

Pa rapòte nan sous revize

Pa gen pitting anba bouyi

C276

ASME Seksyon VIII Div. 1 limit

427 degre (800 degre F)

677 degre (1250 degre F)

C276

Dansite

8.05 g/cm³

8.89 g / cm³

Alyaj 31 (9% pi lejè)

Pri materyèl bwit-(esk.)

~US$10.70/kg

~US$21.40/kg

Alyaj 31 (apeprè mwatye)

Sous: VDM Metals done fèy [1]; Agarwal/Austral Wright [2]; Haynes Entènasyonal [3]. Liy pri se yon kalkil EETA (gade Seksyon 6).

 

Ki sa ki fè yon anviwonman "fòtman oksidasyon," e poukisa li enpòtan?

 

Yon anviwònman ki fòtman oksidan retire elektwon nan metal agresif, epi sèlman alyaj ki gen anpil chromium ka kenbe.Bouyi asid nitrique, asid kwomik, asid ki kontamine ak iyon ferrik oswa kuprik, ak likè klowòks dyoksid klò tout tonbe nan gwoup sa a.

 

Isit la se vèsyon an senp. Nerjaveèi asye ak alyaj nikèl siviv paske chromium fòme yon mens, po oksid envizib. Nan asid modere po sa a pwoteje metal la. Nan asid ki gen anpil oksidasyon, yon chromium -po pòv fonn. Molybdène travay yon fason diferan. Li pwoteje kont diminye asid tankou asid idroklorik ak kont klori pitting, men li fè ti kras ede nan asid oksidan.

 

Diferans sa a eksplike pifò konparezon nan atik sa a. Alloy 31 gen plis chromium. C276 gen plis molybdène. Chak alyaj ranport kote eleman prensipal li yo pi enpòtan.

 

Ki jan alyaj 31 ak Hastelloy C276 diferan nan konpozisyon?

 

Alyaj 31se yon alyaj fè-nikèl-kwòm-molybdène ak nitwojèn. C276 se yon alyaj nikèl-molybdène-kwòm ak tengstèn.Alloy 31 gen apeprè mwatye nikèl C276 ak plis ankò Kwòm. C276 gen apeprè de fwa ak yon mwatye molybdène la.

 

Eleman / pwopriyete

Alloy 31 (UNS N08031)

Hastelloy C276 (UNS N10276)

Nikèl

30.0–32.0%

57% (balans)

Kwòm

26.0–28.0%

16%

Molybdène

6.0–7.0%

16%

Fè

Balans (apeprè 32-34%)

5%

Tengstèn

Okenn

4%

Kwiv / Azòt

1.0-1.4% Cu / 0.15-0.25% N

0.5% Cu max / okenn te ajoute

Kabòn

0.015% max

0.01% max

Dansite

8.05 g/cm³

8.89 g / cm³

PRE (jan yo pibliye)

54

69

 

Sous: Fich done VDM Metals, Tablo 2–3 [1]; Haynes International konpozisyon nominal ak pwopriyete fizik [3]; PRE=%Cr + 3.3×%Mo + 30×%N jan yo endike nan Agarwal, Tablo 1 [2].

 

Yon nòt sou PRE.Ekivalan rezistans pitting (PRE) se yon nòt rapid pou rezistans klori pitting. C276 fè nòt ki pi wo (69 kont 54). Men PRE bay molybdène, pa pou Kwòm ki konbat asid oksidan. Se konsa, yon PRE ki pi wo pa vle di yon pi bon alyaj nan asid nitrique. Li tou inyore tengstèn nan C276.

 

Ki alyaj reziste bouyi asid nitrique pi byen?

 

Alloy 31 reziste asid nitrique bouyi pi byen pase C276 nan pwòp done tès pwodiktè yo.Alloy 31 pèdi apeprè 0.1 mm/a nan yon tès asid nitrique bouyi (tip Huey-). C276 pèdi 22.12 mm/y nan bouyi 65% asid nitrique, apeprè 200 fwa plis.

 

Which Alloy Resists Boiling Nitric Acid Better

 

Kondisyon tès la

Alyaj 31 (mm/y)

C276 (mm/a)

Sous

Bouyi asid nitrique, 65-67%

0.1 (dis peryòd 48-h)

22.12 (65%)

[2], [3]

Menm tès, echantiyon soude (alyaj 625 filler)

0.2

Pa rapòte

[2]

65% asid nitrique nan 93 degre

Pa rapòte

2.53

[3]

65% asid nitrique nan 66 degre

Pa rapòte

0.41

[3]

Bouyi 10% asid nitrique

Pa rapòte

0.26

[3]

 

Alloy 31: Agarwal, "High-chromium alloy resists aqueous kowozyon," repwodui pa Austral Wright Metals [2]. C276: Haynes International reyaktif-done laboratwa klas [3].

 

info-1600-720

Figi 1. Pousantaj korozyon asid nitrique. Marin=Alloy 31, wouj=C276. Valè yo soti nan de pwodiktè diferan, kidonk sèvi ak tablo a pou wè gwosè diferans lan, pa pou konsepsyon ekipman yo.

 

Poukisa diferans lan tèlman gwo

 

Asid nitrique se yon oksidan fò. Nan li, fim nan pwoteksyon chromium se sèl bagay ki enpòtan. Alloy 31 gen 27% Kwòm ak C276 gen 16%. Diferans 11-pwen an parèt kòm yon diferans nan to korozyon de lòd grandè nan bouyi a.

 

De opozisyon onèt

 

Tès yo pa idantik.Rezilta Alloy 31 an mwayèn dis peryòd bouyi 48 èdtan. Tablo Haynes la pa endike longè ekspoze a. Toujou konfime ak yon tès koupon nan pwòp asid ou.

 

Ni alyaj se abityèl premye chwa pou asid nitrique pi.Haynes deklare ke asye pur jeneralman gen ase rezistans nan asid nitrique pi, ak chromium -pote alyaj nikèl yo nesesè sèlman lè alogenid oswa asid alojene tou prezan [4]. Alloy 31 gen sans lè asid nitrique rive ansanm ak klori oswa fliyò, tankou nitrique-marinaj idrofluorik, kote Austral Wright rapòte "bon" rezistans [2].

 

Ki jan yo konpare sou klori, pitting, ak kowozyon nan fant?

 

Tou de alyaj reziste atak klori trè byen, epi C276 kenbe kwen an nan tès ki pi sevè asid melanje-.Nan agresif "Green Death" solisyon an, C276 premye twou sèlman nan pwen an bouyi. Nan sèvis kalite dlo lanmè-, Alloy 31 fè byen nan limit tanperati ak klò ki endike yo.

 

Tès

Alyaj 31

Hastelloy C276

ASTM G48 tanperati kritik pitting (CPT)

85 degre (10% FeCl₃; limit tès)

150 degre (asidifye 6% FeCl₃)

ASTM G48 tanperati kritik fant (CCT)

65 degre (10% FeCl₃)

55 degre (asidifye 6% FeCl₃)

Menm tès, Alloy 625 kòm referans

CPT 77.5 degre / CCT 57.5 degre

CPT 100 degre / CCT 40 degre

Lanmò vèt (11.5% H₂SO₄ + 1.2% HCl + 1% FeCl₃ + 1% CuCl₂)

Pa rapòte nan sous revize

Pitting sèlman nan pwen bouyi

Tès dlo lanmè klowò / fant dlo lanmè

Rezistan a 40-45 degre nan 1.5-2 ppm klò; atak ti fant nan 50 degre

Ap koule tankou dlo: pa gen atak nan 180 jou; dlo toujou: atak 0.10-0.13 mm pwofondè

Klori estrès korozyon krak (bouyi 45% MgCl₂)

Fant (pa pwodiktè); pa gen okenn krak nan bouyi 62% CaCl₂ pou 2,000+ h

Pa gen krak nan 1,008 h

 

Sous: Agarwal/Austral Wright, Tablo 4 ak tèks [2]; Haynes Entènasyonal [3]. Pi wo pase 85 degre solisyon an 10% FeCl₃ kraze chimikman, kidonk 85 degre se plafon tès sa a, pa yon pwen echèk.

 

Pa konpare nimewo CPT yo dirèkteman.Gade nan Alloy 625, ki parèt nan tou de sous. Li fè nòt CCT 57.5 degre nan tès klori ferrik 10% ak CCT 40 degre nan tès klori ferrik asidifye 6%. Menm alyaj, solisyon diferan, nimewo diferan. Se konsa, CCT Alloy 31 a nan 65 degre ak C276 a CCT nan 55 degre te soti nan tès diferan epi yo pa ka klase youn kont lòt. Yon bagay ki serye se ke tou de alyaj yo chita nan tèt ranje a pou rezistans klori, e ke C276 pwouve nan solisyon klori asid ki pi grav -.

 

Ki jan yo konpare nan lòt asid ak nan kondisyon soude?

 

Alyaj 31 pi fò nan asid silfirik cho, mwayen -fòs ak nan pwosesis mouye-asid fosfò.C276se byen lwen pi fò nan asid idroklorik.Chwa a dwat depann de ki asid yo nan kouran ou a, pa sou repitasyon alyaj la.

 

Asid

Alyaj 31

Hastelloy C276

Asid idroklorik

<0.13 mm/y up to 8% at room temperature; resistant only to 3% at 80°C

0.46 mm/y nan 10% ak 66 degre; 1.10 mm/y nan 20% ak 79 degre

Asid silfirik, 40%, 100 degre

0.6 mm/a

10 mm/a (tablo konparezon Agarwal)

Asid silfirik, 80%, 100 degre

240 mm/a (aktif)

240 mm/a (aktif)

Pwosesis mouye-asid fosfò (52–54% P₂O₅, enpur)

0.05 mm/y nan 116 degre

Reyaktif -klas 50% asid, bouyi: 0.18 mm/a

Klò diyoksid blanchi

Evalyasyon "eksepsyonèl" pa pwodiktè

Pa kouvri nan sous revize

 

Sous: Agarwal/Austral Wright, Tablo 2–3 [2]; VDM metal [1]; Haynes Entènasyonal [3]. Medya yo diferan ant sous; gade nòt ki anba a.

 

Yon konfli done ki merite konnen.Tablo konparezon Agarwal bay lis C276 nan 4 mm/a nan 20% asid silfirik nan 80 degre. Tablo pwòp reyaktif -Haynes a bay sou 0.05 mm/a a 79 degre pou menm konsantrasyon an. Sa a se yon diferans nan prèske de lòd nan grandè. Kòz la gen anpil chans se kondisyon tès diferan, tankou pite asid ak aere. Se poutèt sa nou trete klasman asid silfirik ant de alyaj yo kòm reklamasyon pwodiktè yo ki bezwen yon sit-espesifik tès, e poukisa diferans asid nitrique fòtman oksidasyon an se konklizyon ki pi serye.

 

Zòn ki afekte soude ak chalè{0}

 

Alyaj 31:Pwofondè korozyon pi wo a 50 µm devlope sèlman apre de a twa èdtan nan "nen" sansibilizasyon (650-700 degre). Plak soude 6 mm pa te montre okenn atak intergranular nan soude a, HAZ oswa metal debaz [2]. VDM deklare ke pa gen tretman chalè pre-soude ni apre-soude nòmalman obligatwa [1].

 

C276:Trè ba kabòn (0.01% max) ak Silisyòm (0.08% max) fè li rezistan nan sansibilizasyon ki gen rapò soude -. Soude metal korode pi vit pase metal fòje, pou egzanp 1.2 mpy kont 0.1 mpy nan 30% asid silfirik nan 66 degre, men rete nan yon seri ekselan [3].

 

Ki jan alyaj 31 ak C276 konpare sou pri?

 

Alloy 31 koute apeprè mwatye otan ke C276 nan matyè premyè, apeprè US $ 10.70 kont US $ 21.40 pou chak kilogram nan alyaj.Diferans lan soti nan nikèl ak molybdène. C276 gen prèske de fwa nikèl la ak de fwa ak yon mwatye molybdène la.

 

How Do Alloy 31 and C276 Compare on Cost

 

Nou kalkile yon pri "konteni-metal": valè sou mache eleman alyaj prensipal yo andedan yon kilogram alyaj. Se pa yon pri moulen. Li montre etaj pri ki tabli pa mache metal yo.

 

Eleman (pri Septanm. 2026)

Alloy 31 pataje

Alyaj 31 US$/kg

C276 pataje

C276 US$/kg

Pri itilize

Nikèl

31%

5.13

57%

9.43

$16.54/kg (LME, septanm. 23)

Kwòm

27%

0.93

16%

0.55

$3.44/kg (Q3 FeCr referans)

Molybdène

6.5%

4.65

16%

11.43

$71.47/kg (FMI/LME, Out. 31)

Total pou chak kg alyaj

 

10.70

 

21.41

C276 se 2.0 × alyaj 31

Total pou chak lit metal

 

86

 

190

Itilize dansite 8.05 vs 8.89 g/cm³

 

Pri: LME nikèl spot indication, Sept. 23, 2026 (metalcharts.org) [5]; Fon Monetè Entènasyonal/LME tach molybdène, Out . 31, 2026 (Cbonds) [6]; Samchrome Ewopeyen referans ferrochrome, Q3 2026, 156 US¢/lb Cr [7]. Konpozisyon ki soti nan tablo 1 pwen mitan; C276 nikèl kòm balans. Kalkil pa EETA; pa yon figi endepandan pibliye. Tengstèn, kwiv, nitwojèn ak fè yo eskli, kidonk total C276 la se yon ti kras discrete.

 

Ki sa sa vle di nan pratik

 

Rapò a 2× se ki estab.Si molybdène gen yon pri a 92,66 $ US/kg (yon pi gwo sitasyon te wè nan dat 21 septanm . 2026), total yo deplase nan apeprè 12,08 USD/kg ak 24,80 USD/kg, toujou apeprè 2 a 1 [8].

 

Molybdène se faktè balanse.Li se 43% nan Alloy 31 a ki genyen -pri metal men 53% nan C276 a, kidonk C276 se plis ekspoze a mouvman pri molybdène.

 

Pwa ede tou.Alloy 31 se apeprè 9% pi lejè pou chak volim inite, ki diminye tonnaj ou achte pou menm volim ekipman an.

 

Pri filler diminye diferans la yon ti kras.Alloy 31 soude ak Alloy 59 filler (ERNiCrMo-13), li menm yon gwo -nikèl, segondè-molybdène fil [1].

 

Yon egzanp reyèl-monn nan.Pwodiktè -otè afilye papye Alloy 31 la rapòte yon plant asid fosfò ki gen anviwon 780 tib echanjeur chalè ki te ekonomize plis pase 100 000 dola ameriken lè w te chwazi Alloy 31 sou Hastelloy G-30 [2]. Trete li kòm yon ilistrasyon, pa yon garanti.

 

Pri sèlman enpòtan si tou de alyaj siviv.Nan -asid- idroklorik ki gen kouran oksidan oswa pi wo a 427 degre, alyaj ki pi bon mache a pa yon opsyon valab. Konpare pri sèlman nan seri a kote tou de yo akseptab.

 

Ki alyaj ki pi fò, ak ki jan yo fabrike?

 

C276 pi fò e li gen yon limit tanperati kòd ki pi wo. Alloy 31 se pi fasil sou bidjè a epi li gen yon fenèt tretman chalè ki pi laj.Tou de byen soude ak file matche oswa plis -alyaj, epi tou de bezwen pratik magazen pwòp, kontwole.

 

Pwopriyete / pratik

Alyaj 31

Hastelloy C276

Sede fòs (0.2%), tanperati chanm, tipik

280 MPa (40.6 ksi)

356 MPa (51.6 ksi)

Fòs rupture, tanperati chanm, tipik

650 MPa (94.3 ksi)

792 MPa (114.9 ksi)

Elongasyon, tipik

40%

61%

ASME VIII Div. 1 tanperati maksimòm

427 degre (800 degre F)

677 degre (1250 degre F)

Lòt apwobasyon

VdTÜV -196 a 550 degre; NACE MR0175 jiska nivo VI

VdTÜV a 450 degre; NACE MR0175/ISO 15156

Solisyon anneal

1150-1180 degre; fre nan plis pase 150 degre / min soti nan 1100 a 500 degre

1121 degre (2050 degre F); pasè dlo

Limit travay frèt anvan re-rekwit

Pi wo pase 15%

7% ekstèn -elongasyon fib oswa plis

Filler soude

Alloy 59 (ERNiCrMo-13) oswa matche FM 31

ERNiCrMo-4 (matche)

Tanperati maksimòm entèpasaj

120 degre (248 degre F)

Pa kouvri nan sous revize

 

Sous: VDM Metals [1]; Haynes Entènasyonal [3]. Valè alyaj 31 yo se pou fèy nan solisyon -kondisyon rkwit (minimòm ASTM B625: 280 MPa sede, 650 MPa rupture, 40% elongasyon). Valè C276 yo tipik pou fèy 2 mm, pa minimòm.

 

Yon pwen magazen-pou Alloy 31.VDM fè remake ke to travay li -redi se byen pi wo pase sa ki komen asye pur austenitic. Sèvi ak vitès koupe ki ba, manje ki fiks ak yon koupe ase pwofon pou jwenn anba kouch ki te fè tèt di anvan an [1]. Haynes bay avètisman menm jan an pou C276 [3].

 

Ki lè ou ta dwe chwazi alyaj 31, ak ki lè ou ta dwe chwazi C276?

 

Chwazi Alloy 31 lè kouran an ap oksidasyon fò ak ti kras oswa pa gen asid idroklorik, ak tanperati konsepsyon an rete nan oswa anba 427 degre. Chwazi C276 lè oksidan fò yo melanje ak asid idroklorik, tanperati a pi wo, oswa anviwònman an se pi grav ki disponib.

 

Chwazi Alloy 31 pou

  • Bouyi oswa cho asid nitrique, ak nitrique-marinaj idrofluorik, kote kontni chromium deside rezilta a.
  • Mouye-pwosesis echanjeur chalè asid fosfò ak evaporatè, ak sèvis asid silfirik ki kontamine ak klori ak iyon oksidan.
  • Klò diyoksid pou lave klowòks, desulfurization gaz lafimen ak refwadisman dlo lanmè klorin nan tanperati a ak limit klò ki anwo yo.
  • Pwojè kote yon pri materyèl anvan tout koreksyon -pi ba apeprè 50% ak yon pwa ki pi ba apeprè 9% deplase bidjè a.

 

Chwazi Hastelloy C276 pou

  • Kouran oksidan ki genyen tou asid idroklorik oswa asid bromwomik nan konsantrasyon ki gen sans.
  • Tanperati konsepsyon ki pi wo pase 427 degre, jiska 677 degre ASME Seksyon VIII Div. 1 limit la.
  • Anviwònman ki pi sevè ak twou fant yo, tankou likè ki gen lamòd{0}}tip Green Death ak dlo lanmè trankil ak pi gwo maj sekirite.
  • Plant milti-pwodwi kote kouran an chanje ak yon sèl alyaj dwe kouvri oksidasyon, rediksyon ak halogen-devwa pote.

 

Chwazi ni lè

Asid la se pi asid nitrique ki pa gen okenn alogen. Haynes fè remake ke asye pur yo anjeneral ase [4], epi yo koute byen lwen mwens pase swa alyaj.

 

Kesyon yo poze souvan

 

K: Èske Alloy 31 pi bon pase Hastelloy C276?

A:Sa depann de asid la. Alloy 31 se pi bon nan asid fòtman oksidan tankou asid nitrique bouyi, paske li gen 27% CHROMIUM kont 16%. C276 se pi bon nan asid idroklorik, nan tanperati ki pi wo a 427 degre, ak nan tès yo pi sevè.

 

K: Èske Alloy 31 pi bon mache pase Hastelloy C276?

A:Wi. Estimasyon septanm 2026 nou an te genyen-metal se apeprè 10,70 USD/kg pou Alloy 31 kont 21,40 USD/kg pou C276, apeprè mwatye. Pri aktyèl moulen yo varye selon fòm pwodwi, gwosè lòd ak founisè.

 

K: Èske yo ka itilize Alloy 31 nan asid nitrique?

A:Wi. Nan yon tès asid nitrique bouyi (tip Huey-), Alloy 31 pèdi apeprè 0.1 mm / an, ak 0.2 mm / an lè yo soude ak alyaj 625 filler. Pou pi asid nitrique ki pa gen okenn alogen, asye pur se nòmalman chwa ki pi ekonomik.

 

K: Èske Alloy 31 ka ranplase C276 nan asid idroklorik?

A:No Alloy 31 adapte sèlman nan konsantrasyon ki ba asid idroklorik: anba a 0.13 mm / y jiska 8% nan tanperati chanm, epi sèlman nan 3% nan 80 degre. C276 okipe jiska 20% nan tanperati ki wo.

 

K: Ki metal filler yo itilize pou soude Alloy 31?

A:VDM rekòmande Alloy 59 (ERNiCrMo-13, UNS N06059) oswa filler matche FM 31 (N08031). Kenbe tanperati interpass nan oswa pi ba pase 120 degre epi sèvi ak opinyon chalè ki ba.

 

K: Ki tanperati sèvis maksimòm pou chak alyaj?

A:Dapre ASME Seksyon VIII Div. 1, Alloy 31 apwouve a 427 degre (800 degre F) ak C276 a 677 degre (1250 degre F). VdTÜV apwouve Alloy 31 soti nan -196 degre a 550 degre.

 

Ki estanda ki kouvri chak alyaj?

 

Tou de alyaj yo kouvri pa espesifikasyon pwodwi ASTM / ASME ak NACE MR0175 / ISO 15156 pou sèvis tounen.Espesifye klas la pa nimewo UNS sou lòd acha.

 

Fòm pwodwi

Alyaj 31 (N08031)

Hastelloy C276 (N10276)

Plak, fèy, teren

ASTM B625 / ASME SB625

ASTM B575 / ASME SB575

Rod ak ba

ASTM B581, B649 / ASME SB581, SB649

ASTM B574 / ASME SB574

Tiyo ak tib san pwoblèm / soude

Pa nan lis nan tablo VDM revize a

ASTM B622 (san pwoblèm), B619 (soude)

Fittings ak forgings

Pa nan lis nan tablo VDM revize a

ASTM B366 (fittings), B564 (forgings)

Filler soude

ERNiCrMo-13 (Alyaj 59) oswa FM 31

ERNiCrMo-4 / ENiCrMo-4

Ewopeyen / lòt deziyasyon

EN 1.4562, X1NiCrMoCu32-28-7

DIN 2.4819, NiMo16Cr15W

 

Sous: VDM Metals, Tablo 1 [1]; Haynes Entènasyonal, Espesifikasyon ak Kòd [3]. Konfime edisyon aktyèl la ak disponiblite tiyo/fitting ak founisè ou.

 

Sous

[1] VDM Metals, "VDM® Alloy 31 (Nicrofer 3127 hMo) Fich Done Materyèl No . 4131, Rev. 03," Out 2024.https://www.vdm-metals.com/fileadmin/user_upload/Downloads/Data_Sheets/Data_Sheet_VDM_Alloy_31.pdf

[2] DC Agarwal, "High -Alyaj Kwòm reziste korozyon akeuz," Advanced Materials & Processes, Nov. 2004; repwodui nan Austral Wright Metals, High Chromium Alloy 31 fich done pwodwi.https://www.australwright.com.au/technical-data/alloys/high-performance-alloys/nikel-alloys-high-chromium-alloy-31-n08031/

[3] Haynes International, "HASTELLOY® C-276 alyaj."https://haynesintl.com/en/alloys/alloy-portfolio/corrosion-rezistan-alloys/hastelloy-c-276/

[4] Haynes International, Gid Kowozyon, "Anviwònman koroziv yo."https://haynesintl.com/en/corrosion-guide/corrosive-environments/

[5] Metalcharts, "Nickel Price Today," LME nikèl, Sept. 23, 2026.https://metalcharts.org/nickel-pri

[6] Cbonds, "Molybdenum, LME spot price (IMF)," Out. 31, 2026.https://cbonds.com/indexes/181099/

[7] SMM, "Samchrome Sets the Reference Point: 156 US Cents/lb for Q3 2026 European Ferrochrome," Out. 6, 2026.https://news.metal.com/en/newscontent/104046674-samchrome-tabli--referans-pwen-156-nou-centslb-for-q3-2026-european

[8] Pri metal chak jou, molybdène, $42.03/lb nan mwa septanm . 21, 2026.https://www.dailymetalprice.com/molybdenum.html

 

Voye rechèch
Vin jwenn nou
Epi kòmanse RFQs ou kounye a.
Kontakte nou